Thermal Properties of Pure Metals

Element
(At 25°C)

Specific Heat, cal/g°C

Coefficient of Linear Expansion, ( x 10^-6 )
(°C)^-1

Thermal Conductivity, watts/cm°C

Aluminum

0.215

25

2.37

Chromium

0.110

6

0.91

Copper

0.092

16.6

3.98

Gold

0.031

14.2

3.15

Nickel

0.106

13

0.899

Platinum

0.032

9

0.73

Silicon

0.17

3

0.835

Titanium

0.125

8.5

0.2

Zinc

0.093

35

1.15